Author/Authors :
Anbia، M. نويسنده , , Derakhshan، M. نويسنده Department of Electrical Engineering, Imam Khomeini International University, Qazvin, Iran , , Dehghan، R. نويسنده Department of Mathematics, Islamic Azad University, Masjed-Solyman Branch, Iran , , Bandarchian، F. نويسنده Research Laboratory of Advanced Materials, Environment Chem. and Green Tech. Dep., Chemistry and Chemical Engineering Research Center of Iran ,
Abstract :
Ordered mesoporous carbon CMK-3 (OMC) have been synthesized using mesoporous SBA-
15 silica as template and modified with cobalt carbonate. Morphologies and surface texturing of materials were
characterized by X-Ray diffraction (XRD), Scanning Electron Microscopy (SEM) and N2 adsorption-desorption
isotherms. The cobalt modified ordered mesoporous carbon were found to have a surface area of 490.06m2/g
and pore volume of 0.42cm3/g. The adsorption behavior of 1, 10-Phenanthroline (OP) and 2, 2ʹ-bipyridine
(BP) on cobalt modified ordered mesoporous carbon (Co+2-OMC) were studied in aqueous system. The
parameter such as temperature, contact time and initial OP and BP concentrations was investigated. Batch
adsorption studies demonstrate that the cobalt containing CMK-3 has significant capacity for adsorption of
OP and BP from aqueous solution. The adsorption processes of OP and BP are tested with langmuir and
freundlich isotherm models. According to the langmuir isotherms, the maximum adsorption capacities of OP
and BP on Co+2-OMC were 595 and 500 mg/g, respectively.